V. Pyskov’s practical answer to the provincial amateur stranded without paper: how to make a developing-out (“Velox-type”) chloride paper by hand, from choosing the stock to printing it.
The modern amateur, especially in the provinces, is often wholly cut off from his work by the lack of the most necessary materials: plates and chemicals can still be had in tolerable quality, but with papers things stand almost catastrophically — there are no papers of the right surface and gradation, none of the special foreign grades for ozobrome or bromoil, and even the handicraft papers on the market leave much to be desired. One has to recall the old days, when the photographer made almost everything himself, from the negative material to the positive paper — and the work only gained, for a conscious hand is the pledge of success. Making a few sheets oneself brings, besides the creative pleasure, two real advantages: one can change the gradation (a soft- or hard-printing emulsion to suit one’s negatives) and get any surface (matte, velvety, glossy) and thickness (from writing paper to Whatman). The whole process falls into five parts — I. choice and preparation of the paper; II. preparation of the light-sensitive emulsion; III. coating the paper; IV. drying; V. sorting, cutting and packing.
1. Choice and preparation of the paper
If the paper is not to be stored — used up in 2–3 days — and is of high quality (English or German Whatman, or any pure-rag paper), it needs no preliminary treatment; otherwise treatment is necessary. Choose paper free of black and brown specks, well sized, not too rough: the sizing is tested by drawing a few firm pen-strokes of ink — if the edges stay sharp and the ink does not strike through, the sizing is good. Of grades now easily had, all give good results: 1) Alexandrian (thin and thick — a fine-grained velvety surface); 2) Russian Whatman (semi-matte); 3) “papka” (good, postcard-like, glossy when rolled on glass, but some grades have black specks and blister); 4) “book” (even velvety, almost grainless); 5) “card” (very good, like postcards, but hard to find); 6) “ivory” (choose speckless sheets, coat the smoother side; some are poorly sized); 7) thin bristol (like papka); 8) all fine foreign pure-rag drawing papers (usable untreated, but too dear for amateurs).
Preliminary treatment means laying on a protective layer to isolate the paper from the sensitive layer, since the iron, bronze and copper specks, soluble salts and hyposulphite residues in paper quickly decompose an emulsion laid straight on it, causing specks and stains. One either bathes the paper in the protective solution or lays it on with a wide bristle brush (a “Fleitz” flat brush, 6–8 cm or wider, from any haberdasher), well washed and dried; begin with the brush method. The sub-coating solution: gelatin 5 g, water to 100 cu. cm, 10% chrome-alum solution 15 drops (chrome alum may be replaced by double the ordinary alum, or 3–5 drops of formalin). Soak the gelatin half an hour, make up to volume, warm in a glass standing in water at 50–60°, stir till dissolved, add the alum by drops. For special whiteness add, before the alum, 20 g of barium sulphate (barite, blanc-fixe) — hard to buy, but makeable at home by precipitating barium chloride with sulphuric acid to a sharply acid reaction, then washing the insoluble sediment 5–6 times until litmus no longer reddens (the 50–60% barium-sulphate paste then added, 40 cu. cm, to the recipe); barite gives a rust-free paper of bright, lasting whites.
Work in a well-lit room (if evening, the light to the left, no higher than 3/4 m over the table); lay the sheet on 2–3 clean sheets, pin only the top edge (the whole sheet would stretch and wrinkle), hold the bottom with the left hand. Brush the mass on in strokes, first along then across, then level it — pressing hard at first, then ever lighter — until the stripes vanish; hang about half an hour to dry. The recipe suffices for 10–12 sheets of 30×40 cm; the sheets keep indefinitely if kept from dust and damp, stored flat, layer to layer, in a folder or big book (not rolled, as they then crack). This gives a velvety surface. For a matte surface sub-coat instead with spirit (even wood-spirit) 100 cu. cm, rosin or sandarac 5 g, floating the paper 2–5 minutes by its thickness. For a bath that keeps the paper’s natural surface: acetone (or amyl-acetate, or acetic ether) 100 cu. cm, celluloid 5 g (celluloid is got simply by washing the emulsion off old film in boiling water).
2. Preparing the light-sensitive emulsion
The emulsion is chloro-silver, and — to spare the amateur without special gear the difficult washing — it is not washed. One needs two (chemical) glasses, two glass rods, a thermometer, a pot for hot water, and a quarter-arshin of flannel or washed linen; and, of chemicals, silver nitrate (lapis), sodium chloride (table salt), ordinary food gelatin, and chrome or ordinary alum (double the amount of the latter). Gelatin quality matters; special photographic grades being scarce, ordinary food gelatin may be purified thus: swell 100 g in 1000 cu. cm of water (distilled, or boiled and cooled) for 1–1½ hours, heat in a water-bath (never on bare flame — fig. 2) to 70–80°, stirring; at 40–45° it dissolves, then pour in the white of one egg, stirring hard — it curdles into flakes and carries off the impurities; warm 10–15 minutes, let stand 5–10, filter, add 10–15 drops of carbolic acid and set overnight in the cool to a firm jelly. Next day cut away the top quarter and the bottom, keeping the clean middle — about ½ litre of 10% gelatin. This full purifying is only for very dirty, fatty gelatin; if fairly clean, a 10% solution set and trimmed suffices; and clear transparent leaves may be used untreated — the author has often made good emulsions straight from commercial food gelatin.
Then prepare, with ordinary gelatin, solution I: water 370 cu. cm, gelatin 34 g, sodium chloride 20 g; or, with the purified gelatin, gelatin solution 340 cu. cm, water 30, sodium chloride 20 g. And solution II: water 40 cu. cm, silver nitrate 5 g. Heat solution I in the water-bath to 50°, solution II to room temperature (if non-distilled water makes it opalescent, 2–5 drops of 10% nitric acid will clear it, or leave it). In a dark room, under red light, pour solution II into I, stirring; it turns milky and is, strictly, ready to coat — but would work slowly and very hard, so for normal sensitivity and gradation it must be “ripened”: keep it in the water-bath at 50–55° for ½ hour to 3–4 hours, the sensitivity rising (20–30 times) and the working ever softer. Too long or too hot a ripening fogs it; the safe time depends on the gelatin — up to 10–12 hours with true photographic gelatin, but usually 1½–2 hours with food gelatin. Then filter through flannel, add 5 cu. cm of 10% chrome-alum to toughen the layer, and cool to 30–35°; this and all later work is done in the dark room under laboratory light.
3. Coating the emulsion
Of several methods, the beginner should start with the first, which always succeeds, and pass to the faster ones only with experience. First (Melodiev’s) method: on an even table set a tray of hot water the size of the sheet, cover it with a larger glass levelled strictly horizontal (an 18×24 cm tray takes 24×30 cm glass), and on that a second glass of the same size for the actual coating (fig. 3). Soak the sheet 10–15 minutes, roll it onto the upper glass with a rubber roller (or lay it wet, cover with good filter paper and rub well); the warm water heats the glass and paper, and the right amount of emulsion poured on the middle spreads over the sheet — helped if need be with a glass rod or clean finger, the bubbles burst by a fingertip. When the sheet is evenly covered, slide the upper glass off with the paper onto a flat surface, put another glass on the tray, and coat the next sheet; by the time the second is done the first has set (test the edge with a finger), and it is lifted by the corners and hung to dry on a cord with ordinary clothes-pins (fig. 4) — coated in the evening, dry by morning. Emulsion needed: 24×30 cm — 60 cu. cm; 18×24 — 30; 13×18 — 15–20 (increase by about a quarter if hard to spread). When dry, cut to format, reject the bad sheets, fold the good ones layer to layer in waxed or paraffined paper, then black plate-paper, then an envelope or white wrapper under a light press (e.g. between books).
Second method: make a lath frame the size of the sheet and fit into it a slightly larger plywood board so it bows; bend the dry sheet’s edges up like a baking-tray (fig. 6) and lay it in to match the bow (fig. 5). Pour the emulsion into a faience or porcelain teapot, tilt the frame, pour onto one edge (the excess runs back, so the quantity does not matter), and tilt the frame the other way (fig. 7) so the emulsion sweeps evenly across; drain the excess, stand the frame nearly vertical till it stops dripping, and take the sheet to dry. This coats dry paper, greatly speeding the drying and the work — one person can coat and hang 150–200 sheets of 50×60 cm a day — but it needs much skill. Third method: draw the paper through the emulsion with a wooden roller (clear from fig. 8).
4. Printing and development
Since the paper’s character depends on the ripening, no exact exposure can be given; as a guide, a normal negative at 25–30 cm from a 32-candle lamp takes 30–40 seconds. Any developer serves, diluted by half and given 3–5 drops of 10% potassium bromide per 100 cu. cm. A recommended one, giving a bluish-black tone at correct exposure:
| Constituent | Amount |
|---|---|
| Water | 100 cu. cm |
| Metol | 0.1 g |
| Sulphite | 4 g |
| Hydroquinone | 0.4 g |
| Soda | 4 g |
| Potassium bromide, 10% | 1–2 drops |
Fix preferably in an acid alum fixer, though a plain 20% hyposulphite will do; lengthen the fixing to 10–15 minutes, since the hand-coated layer is thicker than a factory one and the fixer needs time to penetrate. Then wash and dry as usual. The paper tones easily with copper baths and to sepia. Emulsion coated on fine-grained paper (Alexandrian, papka, card) can, after washing, be squeegeed for drying onto mirror glass first rubbed with benzine 100, beeswax 1 (a few drops rubbed over the glass with cotton till the streaks go); when dry — and drying may take 1½–2 days, not to be hurried by heat or by lifting the print too soon — the print comes away with a very high mirror gloss.
— V. Pyskov