A new variant of toning bromide papers (“Die Photographische Industrie”)

Bennett published a new variant of toning bromide papers, with preliminary bleaching. Two stock solutions are prepared: I — ammonium bromide 11 g, red prussiate 35 g, water 1000 cu. cm; II — sublimate (a poison!) 28 g, potassium bromide 8 g, hot water 1000 cu. cm. These solutions can keep a long time and serve for the bleaching of bromo-silver copies. Two further solutions serve for the subsequent toning: I — sodium sulphide 330 g, anhydrous sodium sulphite 65 g, water 1000 cu. cm; II — Schlippe’s salt (sulpho-antimony-sodium salt) 10 g, water 1000 cu. cm. Applying the following table of the variation of the given solutions, one can get tones from black to red. The order of work is the usual: a well-washed print is bleached, again well washed, and coloured in the chosen toning bath.

ToneBleaching bathToning bath
BlackSolution I — 1 part + II — 1 partI
Black-brown" 2 parts + 1 part"
Deep-brown" 3 parts + 1 part" (without solution II)
Dark-brown" 5 to 7 parts + 1 part"
Warm-brown" (without bath II)"
Reddish-brown"I — 1 part + II — 7 parts
Red-brown"I — 1 part + II — 4 parts
Red"II (without solution I)

A special developer for negatives with big contrasts (“Revue Française de Photographie”)

At the shooting of manuscripts, drawings, pictures, or at the wish to have a negative with significantly expressed contrasts, it is better to apply for development developers specially composed for this aim. In general features the latter differ from ordinary developers either by another ratio of metol and hydroquinone, or by a bigger quantity of potassium bromide. This developer is very useful also for the development of bromide papers, when it is necessary to get a strong and expressive copy from a flat negative. I. Hydroquinone developer: I — water 1000 cu. cm, potassium metabisulphite 25 g, hydroquinone 25 g, potassium bromide 25 g; II — water 1000 cu. cm, caustic soda 50 g. For development mix solutions I and II in equal parts. II. Metol-hydroquinone developer: water 1000 cu. cm, metol 1 g, anhydrous sulphite 75 g, hydroquinone 9 g, potash 25 g, potassium bromide 5 g.

A metol developer for paper (“Photographische Chronik”)

For getting soft copies on bromide papers, “Photographische Chronik” recommends a pure metol developer: boiled and cooled water 1000 cu. cm, metol 7 g, anhydrous sulphite 35 g, potash 33 g, 10% potassium bromide solution 8 drops. The developer is used without dilution with water, and only in case of the wish to get an especially soft effect it is diluted to a half with water.

The preparation of matte lacquer (“Photographische Chronik”)

“Photographische Chronik” describes the method of preparing matte lacquer recommended by Namias. This method deserves attention by its simplicity and gives in the result a lacquer fine-grained and easily lying on the surface. In 20 cu. cm of ether 1 gram of dammar resin is dissolved. As soon as the solution, after shaking, grows cloudy, there is added to it from a dropper 20–30 drops of alcohol (not more than 1 cu. cm). After the lacquer has stood some time and become light, it can be put to use.

— N. D. Petrov

Bubbles on photographic prints

The bubbles appearing sometimes on photographic prints owe their appearance for the most part not to the quality of the paper, but to the wrong manipulations on the part of the photographers. Bubbles can appear during development, fixing, toning and washing. Very rarely do bubbles appear during development; far more often during fixing, especially if the developer was too alkaline and the fixer too acid, or if prints from an alkaline developer are lowered into an acid fixer without preliminary rinsing with water. The carbon-dioxide gas forming in the thickness of the swollen gelatin layer tears the gelatin from the paper backing and forms bubbles. Hence the rules: 1) if possible, not to use too alkaline a developer and too acid a fixer; 2) after development, before lowering into the fixer, to rinse the prints without fail in water. In water there is always dissolved a certain quantity of air, and if the surrounding temperature begins to rise, the air is released from the water and raises the gelatin, giving bubbles; this phenomenon can be prevented by tanning the gelatin layer; hence rule 3): in the hot time of the year to use only an acid tanning fixer. One should avoid too sharp fluctuations of temperature at the transfer of prints from one bath to another (for example, from a cold washing after the developer into a warm fixer); this happens usually in winter; hence rule 4): the temperature of all the solutions should, if possible, be the same; and 5): in winter fix prints in a bath having the temperature of the washing water. Bubbles at washing can appear in those places where the bond between the gelatin layer and the backing is disturbed by pressure or displacement; hence rule 6): not to touch the prints (especially in hot weather) once more with the fingers, not to fix negatives together with prints, and not to let a strong jet of water onto the prints. If during the final washing bubbles have appeared, then behind each of them one should prick the paper backing with a thin needle; then at drying the bubbles usually “settle,” and only a narrow, barely noticeable ring remains.

— A. Kolosova