P. Lyadov on the neglected last step — drying the negative. Why long or uneven drying harms the gelatin (and breeds bacteria), how to speed it with a fan of warm air blown parallel to the film, the drying-stand trick for saving space, tanning with alum or formalin, and the right way to dry with spirit.
If it is desirable to get a flawless negative, it is necessary to perform all the required manipulations with it with due attention; to the number of such manipulations relates also the drying of the negative. For this, first of all, a place should be chosen that is aired and free from dust. In the absence of good ventilation, drying takes place very slowly, and with some sorts of gelatin can last up to 1½ days and more — for example, if one leaves the negative for the night in a closed damp premises. Long drying is extremely harmful for gelatin. Besides, in summertime the bacteria developing in the gelatin destroy the latter, as a result of which on the negative small points form. To speed the drying of negatives it is recommended to apply a fan, especially if it acts with heated air. Here the stream of air should act not slantwise, but parallel to the film surface of the negative, so that the dust particles accidentally brought by it should not fall on the gelatin surface. In case drops of water or of some liquid fall on a dried negative, it is necessary at once to put it in water and hold it in it until the whole layer softens, which sometimes requires a prolonged time; the air bubbles sometimes appearing at soaking should be carefully removed with the finger under water.
In order that the drying of negatives, even in unfavourable conditions (damp, cold air and so on), should not drag out especially, one puts the plates in a drying-stand (the so-called “trestles”) with large intervals between them. To save space, one can put every two plates (glass side to each other) in two consecutively-going slots, leaving between the emulsion surfaces an interval of no less than three slots. Here it is necessary, before putting the plate in the stand, to wipe its glass side dry. In any case, separate drops of water not removed in time from the glass side of the negative will cause at the corresponding places of the gelatin layer a slower drying of the latter. But the main condition of the drying of the negative is the uniformity of the process from beginning to end. If the drying was at first slowed, and then at once sped up, or the reverse, such a sharp transition reflects in greater or lesser degree on the negative, which will have either an uneven density, or, being outwardly good, will reveal an unevenness of the layer at intensification or weakening. To ensure a uniform drying, one should dry the plates all the time at identical atmospheric conditions. At the accumulation on the lower corners of the negative of water drops, causing a slowing of the drying of the plate in these places, such accumulations of water should be removed from time to time. It is also necessary to wipe the water draining from the plates under the drying-stand, so as not to drag out even more the process of drying the plates from below. If it is desirable to speed the drying without the help of a fan, one has to resort to the treatment of the gelatin layer with chemical means, which are, first of all, alum or formalin, whose purpose is, properly, to tan the gelatin layer so that the latter, at some heating of it, should not be able to melt. One should not apply too strong a tanning bath, since from this the layer becomes very fragile and then already cannot well perceive retouch. With film negatives, moreover, in view of the flexibility of the celluloid substrate, a strongly-tanned layer not only gives breaks but easily bounces off the substrate.
At the wish to dry negatives with alcohol, one should use a sufficiently high-percentage spirit. For celluloid films drying with alcohol is not suitable, since from it the film wrinkles. A preliminary alcohol bath speeds the process of the drying of the negative, but often causes a dimming of the layer; this external unseemliness of the negative, in the words of the well-known photo-chemist Lüppo-Cramer, can be removed by the fact that such a quickly-dried negative can, on occasion, again be soaked and then dried already in the normal order.
For economic purposes, for the drying of negatives one should, of course, use denatured spirit, as cheaper and more easily obtained.
— P. Lyadov
About this see “Sovetskoe Foto,” 1927, No. 4, p. 122.