USSRPhoto.com

Soviet Photo Archive / 1928 No. 8

The Making of Photographic Paper

G. K—kh · article · original pages 346–347

G. K—kh’s companion-piece to his No. 7 article on plate-making: how photographic paper is made. The chemically-pure rag base bought by the roll from Germany; why it must never touch metal rollers; the baryta sub-layer that gives strength, gloss and whiteness; the 500-metre coating, calendering under 20,000 kg, and emulsion-spraying machines; and the ways the paper emulsion differs from the plate emulsion.

Still comparatively recently, when we fed exclusively on imported photo-paper, its making seemed to us a matter well-nigh superhuman. At present, when the market is heaped with paper of handicraft production — made by everyone too lazy to do otherwise, and everyone who was unlucky in other branches of activity — we fall into the other extreme, and are ready to consider the making of paper equivalent to the baking of rolls and the sewing of boots. Both the one and the other is, understandably, incorrect.

The production of paper, just as of plates, is a very complex process, requiring great knowledge, experience and special, very complex equipment. No small role is played by external conditions too: just as in plate production, pedantic cleanliness is observed; the factories are placed in parks outside the town, or supplied with various complex devices for ventilation and the cleaning of the air from the slightest dust. All the materials and raw stuff used must be of the first grade and chemically absolutely pure. Only with all these conditions present can one get a product of high quality. Here lies the secret of the advantage of the world firms, with their old accumulated experience, highly-qualified scientific labour-force, newest mechanical equipment and standard raw material.

The base and the baryta layer

The paper proper, or, as they call it, the base, a rare factory makes itself — in most cases it is got ready from special factories in the form of enormous rolls. In Germany there are two such factories. The paper intended for coating with emulsion must not contain in its composition any substances which could enter into a harmful reaction with the substances of the emulsion; it must be chemically pure, and the antichlor used at bleaching must be thoroughly removed from it. Rag paper, without any admixture of wood, is preferred, since the latter harmfully influences the colouring. It is very important that at the processing of the paper it should not be passed through metal rollers, since microscopic particles of metal getting in subsequently destroy the light-sensitive layer and give on the prints points of various colours. Insufficiently sized paper does not have the needed strength, deforms at processing (whence a distorted print results), and its porosity absorbs the emulsion (whence the richness of the image suffers).

But even the very best paper is unfit for the direct covering with emulsion. Firstly, it does not have a sufficiently even and tender surface; and secondly, coming into direct contact with the emulsion, it quickly decomposes it, in consequence of which such paper does not withstand any prolonged storage. The only way out is the application on the paper of an intermediate insulating sub-layer of some neutral substances. Most of all for this purpose is used barium sulphate in a mixture with the neutral binding substance gelatin; and this very process is called baryta-coating. The advantage of a baryta layer is strength, cleanliness, gloss and whiteness. For papers with a visible image, instead of gelatin they sometimes take agar-agar and add a whole series of other substances: glycerine, spirit, milk, chrome-alum, citric acid and so on; sometimes, for colour, they add a little weakly-pink or pale-violet paint. All the substances intended for the composition of the baryta mass are ground into the finest dust in special machines — mills and mixers — the peculiarity of which consists in that the chemicals do not come into contact with any metal parts of the mechanism. After grinding and mixing, the powder enters a sieving machine, where by special brushes it is rubbed through very dense sieves; after this, by dilution with water, it is brought to a paste-like state and in this form used for application to the paper.

The application of the baryta layer is produced on special baryta-coating machines resembling those used in wallpaper production. The construction of such machines gives the possibility of processing a ribbon of paper 500 metres long in premises 30 metres long and 4 metres wide. The drying is produced at a moderate temperature. The dried paper enters a winding machine which rolls it into a roll; to this machine are attached knives for levelling the edges and an automatic measuring device. The process of baryta-coating is sometimes repeated several times to attain the proper result. After baryta-coating the paper passes through a moistening machine where, by a blast of air, moisture is distributed over its whole surface in an exactly regulated quantity; then it is passed through a calender where it is subjected to presses with a pressure of 20,000 kilograms, thanks to which its surface becomes completely smooth. Rolled again into a roll by another, more energetically acting, winding machine, the paper is ready for the coating with emulsion. But before that it is subjected to a comprehensive analysis: the weighing of one square metre, the evenness of its covering, tearability, whiteness, gloss and so on. Trial coatings are made, and only after establishing conformity to the standard is it recognised fit for further work.

The paper emulsion and the coating

On the making of the emulsion we shall not stop here, since we set it out in sufficient detail in our article on plates — in No. 7 of “Sovetskoe Foto”; we shall say only a few words of the difference from the plate emulsion. For bromide papers harder sorts of gelatin are taken. The ripening of the emulsion is conducted sometimes without ammonia, and goes weaker than in the plate one. To the chloro-bromo-silver, so-called “gaslight” paper, is given a comparatively weak ripening, without ammonia, at a temperature of 40–50° Celsius. Especially carefully is conducted the ripening of the emulsions for low-sensitivity papers of this type with a blue-black tone, since they easily over-ripen and fog. For some sorts of emulsion the order of “mixing” changes: instead of pouring silver nitrate into the gelatin solution with the halides, they pour the halides into the gelatin solution with the silver nitrate. The influence on gradation is attained by the addition of potassium iodide at various periods of the ripening. Besides gelatin emulsions, collodion ones are used (for celloidin papers), albumin ones and so on. In all the rest the work is conducted the same as in the plate emulsion. Some emulsions of “gaslight” papers go to coating immediately on ripening, without subsequent washing; such simplified emulsions are composed rather quickly and go mainly for the making of cheap, contrastily-working papers. Matte and semi-matte surfaces are attained by the addition of starch to the emulsion in various combinations.

[Figure: a scheme of the coating and drying of paper.]

The coating of papers with emulsion is produced on special coating machines, the construction of which depends on the kind of emulsion and its temperature at coating. For bromo-silver, chloro-bromo-silver and aristotype papers a gelatin emulsion is used, coated in a melted state. From a large roll the paper is unwound and passes through the machine; thanks to a whole system of braking and regulating devices, its movement proceeds evenly. The covering with emulsion is produced in the machine by a special spraying device acting by air-pressure; this device is connected with a heated vessel in which the melted emulsion is, and the sprayer acts evenly over the whole width of the paper. With the machine is inseparably connected a cooling device assisting the quicker congealing of the emulsion coated on the paper (ice, cold water or a current of cold air). The drying of the paper is produced by a current of warm air carefully cleaned beforehand of dust. The metal parts of the winder are covered with soft, chemically-harmless material. The emulsion layer is sometimes covered also with a protective layer of tanned gelatin; by this same means are got on the paper certain surfaces which by another method cannot be got.

We shall not stop here on how the dried paper, before entering the warehouse, is carefully analysed, controlled, sorted, cut into the needed formats and packed. All this was described in detail in our article on the making of plates — the principle and the methods are the same.

— G. K—kh