N. D. Petrov explains the halo — the superfluous blackening around a bright point, caused by light that passes the emulsion, reflects off the back of the glass and returns to the layer — and why it grows toward the plate’s edges and with glass thickness. Then the remedies, from least to best: short development, loading the plate emulsion-inward, the double-emulsion “Sandell” plate, a non-actinic backing (two home recipes — a gelatin-glycerine-aniline paper and Helain’s soot-dextrin paint), and — the best — a coloured intermediate layer (Agfa “Chromo-Isolar”); closing with Rheden’s table showing that ordinary films are barely better than ordinary plates.
At the shooting of bright or contrastly-lit objects there is sometimes the necessity of long exposing the plate, exposing for the shadows. During this time the light rays act on the light-sensitive layer and, refracting, enter the thickness of the glass; having passed it, part of the rays is absorbed by the black surface of the cassette wall, and some other part reflects from the glass side of the plate and again falls at some point on the light-sensitive layer. Thus one and the same ray produces an impression on the sensitive layer twice: at its falling along the line ABO, and, having reflected elsewhere, at the point “o.” Taking into account the insignificant thickness of the sensitive layer, and excluding reflection from the cassette wall (which should be black-matte), we may say that at these points the light-action expresses itself at development by the restoration of silver bromide (blackening). In other words, all reflected rays of the character “ABO” and “aBO¹” give around the point “B” a completely superfluous blackening at the points “o” and “o¹” — the phenomenon it is accepted to call a halo (Fig. 1).
The distances “Oo” and “O¹o¹,” the width of the halo around “B,” depend on two causes: the angle of incidence of the ray on the plate, and the length of the perpendiculars “BG” (the thickness of the glass). The ray “aB,” forming with the plate an angle closer to a right one than “AB,” gives a smaller halo, since “O¹o¹” is less than “Oo.” As the rays like “AB” fall nearer the edges of the plate and those like “aB” nearer its middle, one concludes: the danger of haloes increases from the middle of the plate toward its edges, where they can be very significant. And at a decrease in the thickness of the glass, the danger of haloes is less.
The remedies
A few words first about the role of the duration of development. If development lasts long, the developer penetrates through the whole emulsion layer; and since the light-action of the reflected rays begins from its lower layers, this penetration emphasises the halo. So the first device suggests itself — to develop the plate not long, not working the image through completely; correct in sense, but coupled in practice with a large risk of an unworked, flaccid negative (at least with the usual development).
Sometimes, to avoid haloes, the plate is placed in the cassette with the light-sensitive layer inward. The image then comes out reversed (not always convenient); and the emulsion side is taken out of the plane of the ground glass on which focus was made, so to preserve sharpness one must, after focusing, move the ground glass toward the lens (shorten the bellows) by the thickness of the glass. This trick still does not exclude haloes.
Some German firms release plates whose sensitive layer is in two rows: the first, coated on the glass, is an emulsion of very low sensitivity, the upper of high sensitivity (the Sandell-platte). Here haloes are unconditionally fewer, since the light-impressions of the reflected rays are received first by the low-sensitivity layer.
More interesting are the methods that destroy the very possibility of reflection from the glass side — the origin of the factory anti-halo plates. Covering the reverse side with a non-actinic paint holds back much of the actinic rays; foreign firms sometimes use instead a thin coloured film; both wash off at development. A home-made backing: cover a thin but strong paper with an even brushed layer of — Water 30 cu. cm, Gelatin 4 g, Glycerine 24 cu. cm — plus red aniline paint enough to colour the whole mixture intensively (dissolve the gelatin in a water bath, add the water and glycerine, then saturate with paint); cut the sticky paper into formats and press it to the glass side with a rubber roller (at red light); before development it peels off easily, and after rubbing with glycerine can serve again. A second method applies paint directly to the glass, by Helain’s recipe (1901): fine soot in powder 10–12 g, yellow dextrin 100 g, ammonium chloride (sal-ammoniac) 6 g, water 90–100 cu. cm — moisten the soot with a little denatured spirit, add the dextrin, pour in the water with the dissolved sal-ammoniac, grind to uniformity with a spatula and leave a day; apply with a wide bristle brush at dim red light, dry about 3 hours in darkness; before development it washes off in water.
The best method places between the sensitive layer and the glass a special intermediate, non-actinically-coloured layer absorbing the rays that have passed the emulsion: the rays’ actinic part is held on entering the glass, and again on reflecting back through the layer, so the light-impression of the reflected rays is so insignificant that haloes can be considered practically destroyed. Typical of such plates are the German “Agfa” “Chromo-Isolar.”
In conclusion, the results of the latest laboratory experiments of I. Rheden with anti-halo plates of various types. If the minimum exposure needed for the visible blackening of the plate is taken as unity, then the number of units needed to form haloes can be reduced to this table:
| Ordinary plates and films | 100–500 |
| Plates with double emulsion (Sandell-platte) | 500–2,000 |
| Plates with a coloured reverse side | about 2,000 |
| Plates with a coloured intermediate layer (“Chromo-Isolar” type) | 5,000–70,000 |
These practically very valuable conclusions are interesting also in that the widespread opinion about the anti-halo quality of films is refuted by Rheden’s researches: ordinary films, in the sense of anti-halo quality, present compared with the same plates only a slight advantage, but by no means more.
— N. D. Petrov